陶氏公司利用HT-GPC-IR和CEF设备开发高性能聚烯烃材料产品和方法
陶氏 Dow Global Technologies LLC公司利用现代聚烯烃表征技术高温凝胶渗透色谱法HT-GPC-IR和CEF(结晶淋洗分级技术)设备开发高性能聚烯烃材料。相关的新材料和制造专*利技术“改性聚乙烯组合物及其制造方法”已申请美国专*利并正式公开。


HT-GPC-IR CEF
以下是该专*利的相关摘要介绍。
摘 要
专*利名:MODIFIED POLYETHYLENE COMPOSITIONS AND METHOD FOR MAKING THE SAME
改性聚乙烯组合物及其制造方法
申请人Applicant: 陶氏 Dow Global Technologies LLC (Midland, MI); PBBPolisur S.R.L. (City Of Buenos Aires, AR)
专*利号:US 20200239673 A1
公开日期:July 30, 2020
专*利摘要:
一种提高聚乙烯树脂的熔体强度和/或降低剪切粘度的方法,该方法包括:
- 提供一种包含乙烯和任选的一种或多种α-烯烃共聚单体的聚乙烯组合物,该聚乙烯组合物表征为以下的各种性质:密度范围为0.900g/cm.sup.3至0.970g/cm.sup.3,分子量分布(Mw/Mn)范围为2.6至3.5,以及每1,000个总碳原子中含0.10至0.27个乙烯基;b) 提供包含自由基产生剂和聚乙烯树脂的母料组合物,其中自由基产生剂在220°C下的半衰期小于200秒,且分解能高于-250kJ/mol,其中,所述聚乙烯树脂的密度为0.900g/cm.3至0.970g/cm.3,熔融指数为0.01g/10min至100g/10min;和c) 使聚乙烯组合物与母料组合物反应以形成改性聚乙烯组合物。
在该专*利技术的开发过程中,采用了Gel permeation chromatography (GPC) 和Crystallization Elution Fractionation(CEF)两种聚烯烃微观结构表征技术。
ABSTRACT
A method for increasing the melt strength and/or low shear viscosity of a polyethylene resin, the method comprising a) providing a polyethylene composition comprising the reaction product of ethylene and optionally, one or more alpha-olefin comonomers, wherein the polyethylene composition is characterized by the following properties: a density ranging from 0.900 g/cm.sup.3 to 0.970 g/cm.sup.3, a molecular weight distribution (Mw/Mn) ranging from 2.6 to 3.5, and from 0.10 to 0.27 vinyl groups per 1,000 total carbon atoms; b) providing a masterbatch composition comprising a free radical generator and a polyethylene resin, wherein the free radical generator has a half-life at 220 C of less than 200 seconds, and a decomposition energy higher than −250 kJ/mol, and wherein the polyethylene resin has a density ranging from 0.900 g/cm.sup.3 to 0.970 g/cm.sup.3, melt index ranging from 0.01 g/10 min to 100 g/10 min; and c) reacting the polyethylene composition with the masterbatch composition to form a modified polyethylene composition.
技术领域
本公开的实施方案总体上涉及制造具有增加的熔体强度和/或低剪切粘度的改性聚乙烯组合物的方法。
TECHNICAL FIELD
[0001] Embodiments of the present disclosure generally relate to methods of manufacturing modified polyethylene compositions having increased melt strength and/or low shear viscosity.
研发背景
聚乙烯树脂在许多方面的应用都需要良好物理性能、易于加工以及用于形成薄膜或吹塑制品时的足够熔体强度和/或收缩张力。
线性低密度聚乙烯 (LLDPE) 具有非常理想的物理性能,但可能缺乏足够的熔体强度和/或收缩张力,无法用于某些薄膜应用,例如大气泡膜、整理收缩膜,或吹塑应用、管道应用和挤出涂层应用。
在许多应用中,LLDPE 与 LDPE 的共混物用于提高加工过程中的 LLDPE 熔体强度和/或加工所得薄膜的收缩张力。或者,可以通过增加LLDPE的分子量的方式来增加LLDPE熔体强度。然而,此类解决方案可能会带来挑战。例如,高分子量的LLDPE会导致较高的挤出压力,从而降低挤出产量并可能导致熔体破裂。
典型的解决方案可能是添加一定量的 LDPE,根据应用要求,添加量从 20% 到 60% 不等,以提高工艺稳定性;然而,添加 LDPE 会导致机械性能显着下降,例如抗撕裂、穿刺和落镖冲击阻力性能。
因此,需要一种替代方法,用来生产具有增加的熔体强度和/或低剪切粘度的聚乙烯组合物。
BACKGROUND
[0002] Polyethylene resins are used in many applications requiring good physical properties, easy processing, and sufficient melt strength and/or shrink tension for formation of films or blow molded articles. Linear Low Density Polyethylene (LLDPE) has very desirable physical properties, but may lack sufficient melt strength and/or shrink tension to be used in certain film applications, such as, large bubble films, collation shrink films, or in blow molding applications, pipe applications, and extrusion coating applications. In many applications, a blend of LLDPE with LDPE is used to increase the LLDPE melt strength during processing and/or shrink tension of resultant films. Alternatively, LLDPE melt strength may be increased by increasing the molecular weight of the LLDPE. Such solutions, however, can present challenges. For example, LLDPE with high molecular weight can cause high extrusion pressure, thereby lowering extrusion output and potentially causing melt fracture. A typical solution may be to add an amount of LDPE, varying from 20 to 60% depending on the application requirements, to improve process stability; however, the addition of LDPE can cause a significant drop in the mechanical properties, such as, tear, puncture, and dart impact resistance.
[0003] Accordingly, alternative methods for producing polyethylene compositions having increased melt strength and/or low shear viscosity are desired.
本专*利技术研发过程中采用的两种聚烯烃微观结构表征技术:
Test Methods 测试技术
Crystallization Elution Fractionation (CEF) Method
[0071] The Crystallization Elution Fractionation (CEF) technology is conducted according to Monrabal et al, Macromol. Symp. 257, 71-79 (2007). The CEF instrument is equipped with an IR-4 or IR-5 detector (such as that sold commercially from PolymerChar, Spain) and a two angle light scattering detector Model 2040 (such as those sold commercially from Precision Detectors). A 10 micron guard column of 50 mm×4.6 mm (such as that sold commercially from PolymerLabs) is installed before the IR-4 or IR-5 detector in the detector oven. Ortho-dichlorobenzene (ODCB, 99% anhydrous grade) and 2,5-di-tert-butyl-4-methylphenol (BHT) (such as commercially available from Sigma-Aldrich) are obtained. Silica gel 40 (particle size 0.2-0.5 mm) (such as commercially available from EMD Chemicals) is also obtained. The silica gel is dried in a vacuum oven at 160° C. for at least two hours before use. ODCB is sparged with dried nitrogen (N.sub.2) for one hour before use. Dried nitrogen is obtained by passing nitrogen at <90 psig over CaCO3 and 5 Å molecular sieves. ODCB is further dried by adding five grams of the dried silica to two liters of ODCB or by pumping through a column or columns packed with dried silica between 0.1 ml/min to 1.0 ml/min Eight hundred milligrams of BHT are added to two liters of ODCB if no inert gas such as N.sub.2 is used in purging the sample vial. Dried ODCB with or without BHT is hereinafter referred to as “ODCB-m.” A sample solution is prepared by, using the autosampler, dissolving a polymer sample in ODCB-m at 4 mg/ml under shaking at 160° C. for 2 hours. 300 μL of the sample solution is injected into the column. The temperature profile of CEF is: crystallization at 3° C./min from 110° C. to 30° C., thermal equilibrium at 30° C. for 5 minutes (including Soluble Fraction Elution Time being set as 2 minutes), and elution at 3° C./min from 30° C. to 140° C. The flow rate during crystallization is 0.052 ml/min The flow rate during elution is 0.50 ml/min The IR-4 or IR-5 signal data is collected at one data point/second.
[0072] The CEF column is packed with glass beads at 125 μm±6% (such as those commercially available with acid wash from MO-SCI Specialty Products) with ⅛ inch stainless tubing according to U.S. Pat. No. 8,372,931. The internal liquid volume of the CEF column is between 2.1 ml and 2.3 ml. Temperature calibration is performed by using a mixture of NIST Standard Reference Material linear polyethylene 1475a (1.0 mg/ml) and Eicosane (2 mg/ml) in ODCB-m. The calibration consists of four steps: (1) calculating the delay volume defined as the temperature offset between the measured peak elution temperature of Eicosane minus 30.00° C.; (2) subtracting the temperature offset of the elution temperature from the CEF raw temperature data. It is noted that this temperature offset is a function of experimental conditions, such as elution temperature, elution flow rate, etc.; (3) creating a linear calibration line transforming the elution temperature across a range of 30.00° C. and 140.00° C. such that NIST linear polyethylene 1475a has a peak temperature at 101.00° C., and Eicosane has a peak temperature of 30.00° C., (4) for the soluble fraction measured isothermally at 30° C., the elution temperature is extrapolated linearly by using the elution heating rate of 3° C./min. The reported elution peak temperatures are obtained such that the observed comonomer content calibration curve agrees with those previously reported in U.S. Pat. No. 8,372,931.
Comonomer Distribution Breadth Index (CDBI)
[0073] The CDBI is calculated using the methodology described in WO/93/03093 from data obtained from CEF. CDBI is defined as the weight percent of the polymer molecules having a comonomer content within 50 percent of the median total molar comonomer content. It represents a comparison of the comonomer distribution in the polymer to the comonomer distribution expected for a Bernoullian distribution.
[0074] CEF is used to measure the short chain branching distribution (SCBD) of the polyolefin. A CEF molar comonomer content calibration is performed using 24 reference materials (e.g., polyethylene octene random copolymer and ethylene butene copolymer) with a narrow SCBD having a comonomer mole fraction ranging from 0 to 0.108 and a Mw from 28,400 to 174,000 g/mole. The ln (mole fraction of ethylene), which is the ln (comonomer mole fraction), versus 1/T (K) is obtained, where T is the elution temperature in Kelvin of each reference material. The comonomer distribution of the reference materials is determined using 13C NMR analysis in accordance with techniques described, for example, in U.S. Pat. No. 5,292,845 (Kawasaki, et al.) and by J. C. Randall in Rev. Macromol. Chem. Phys., C29, 201-317.
High Temperature Gel Permeation Chromatography (HT-GPC)
[0078] A PolymerChar (Valencia, Spain) high temperature Gel Permeation Chromatography system consisting of an infra-red concentration detector (IR-5) is used for MW and MWD determination. The solvent delivery pump, the on-line solvent degas device, auto-sampler, and column oven are from Agilent. The column compartment and detector compartment are operated at 150° C. The columns are three PLgel 10 μm Mixed-B, columns (Agilent). The carrier solvent is 1,2,4-trichlorobenzene (TCB) with a flow rate of 1.0 mL/min. Both solvent sources for chromatographic and sample preparation contained 250 ppm of butylated hydroxytoluene (BHT) and are nitrogen sparged. Polyethylene samples are prepared at targeted polymer concentrations of 2 mg/mL by dissolving in TCB at 160° C. for 3 hour on the auto-sampler just prior the injection. The injection volume is 200 μL.
[0079] Calibration of the GPC column set is performed with 21 narrow molecular weight distribution polystyrene standards. The molecular weights of the standards ranged from 580 to 8,400,000 g/mol, and are arranged in 6 “cocktail” mixtures, with at least a decade of separation between individual molecular weights. The polystyrene standard peak molecular weights are converted to polyethylene molecular weights using the following equation (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)):
M.sub.polyethylene=A(M.sub.polystyrene).sup.B
[0080] Here B has a value of 1.0, and the experimentally determined value of A is around 0.42.
[0081] A third order polynomial is used to fit the respective polyethylene-equivalent calibration points obtained from equation (1) to their observed elution volumes. The actual polynomial fit is obtained so as to relate the logarithm of polyethylene equivalent molecular weights to the observed elution volumes (and associated powers) for each polystyrene standard.
[0082] Number-, weight- and z-average molecular weights are calculated according to the following equations:
[00001]Mn_=.Math.i.Math.Wfi.Math.i.Math.(Wfi.Math./.Math.Mi)(2)Mw_=.Math.i.Math.(Wfi*Mi).Math.i.Math.Wfi(3)Mz_=.Math.i.Math.(Wfi*Mi2).Math.i.Math.(Wfi*Mi)(4)
Where, Wf.sub.i is the weight fraction of the i-th component and M.sub.i is the molecular weight of the i-th component. The MWD is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn).
[0083] The accurate A value is determined by adjusting A value in equation (1) until Mw, the weight average molecular weight calculated using equation (3) and the corresponding retention volume polynomial, agreed with the independently determined value of Mw obtained in accordance with the linear homopolymer reference with known weight average molecular weight of 120,000 g/mol.
注:中文部分如有不清楚的地方,请以原文为准!